<?xml version="1.0"?>
<feed xmlns="http://www.w3.org/2005/Atom" xml:lang="en">
	<id>https://wiki.cmm.uq.edu.au/api.php?action=feedcontributions&amp;feedformat=atom&amp;user=UQdpeace</id>
	<title>CMM Wiki - User contributions [en]</title>
	<link rel="self" type="application/atom+xml" href="https://wiki.cmm.uq.edu.au/api.php?action=feedcontributions&amp;feedformat=atom&amp;user=UQdpeace"/>
	<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Special:Contributions/UQdpeace"/>
	<updated>2026-11-21T22:58:37Z</updated>
	<subtitle>User contributions</subtitle>
	<generator>MediaWiki 1.46.0</generator>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=61</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=61"/>
		<updated>2026-11-13T02:44:16Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: Updated with expanding sections for BEAMER and silicon etching.&lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: &#039;&#039;&#039;1.72 ± 0.21 dB/cm&#039;&#039;&#039; (0.50 µm strip, air-clad).&lt;br /&gt;
&lt;br /&gt;
[[File:SOI220_Standard_Process_Flow.png|left|1200px|220 nm SOI standard process flow]]&lt;br /&gt;
&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
|style=&amp;quot;width:70%; vertical-align:top;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate clean&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry. 5 min dehydration bake at 180 °C, then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma (200 W, 100 sccm O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt;, 10 mTorr).&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood and sonicator&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — Resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; before dispensing.&lt;br /&gt;
&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 3 — Pre-exposure bake&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe &amp;quot;ZEP520A on SOI&amp;quot;).&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
* Filmtek&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 4 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose at 100 kV as two passes from one BEAMER flow (see &#039;&#039;EBL data preparation&#039;&#039; below):&lt;br /&gt;
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step&lt;br /&gt;
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step&lt;br /&gt;
&lt;br /&gt;
* CMM — Raith EBPG5150 (100 kV)&lt;br /&gt;
* Process flow PDF: [[Media:SiCOI litho.pdf|SiCOI litho]] &amp;lt;!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --&amp;gt;&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 5 — Development&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 6 — Resist reflow (optional)&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 7 — Si etch&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see &#039;&#039;Si etch sequence&#039;&#039; below). Si : ZEP selectivity is ~1.55 : 1.&lt;br /&gt;
&lt;br /&gt;
* ANFF-Q — Oxford ICP-RIE&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 8 — Resist removal&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma at 200 W.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood, Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 9 — Inspection&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.&lt;br /&gt;
&lt;br /&gt;
* Optical microscope&lt;br /&gt;
* CMM — Dektak; ANFF-Q — KLA profiler&lt;br /&gt;
* CMM — eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 10 — Dicing&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Coat with AZ protective resist, dice, then solvent clean as in Step 1.&lt;br /&gt;
&lt;br /&gt;
* Sawatec spin coater (protective coat)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
|style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — clean, coat, EBL, metrology&lt;br /&gt;
* ANFF-Q (AIBN) — etch, depth profiling&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150 (100 kV EBL)&lt;br /&gt;
* BEAMER (EBL data preparation)&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
* Oxford ICP-RIE&lt;br /&gt;
* Diener plasma cleaner&lt;br /&gt;
* CEE Apogee spin coater&lt;br /&gt;
* Filmtek (film thickness)&lt;br /&gt;
* Dektak / KLA (step height)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone (standard process)&lt;br /&gt;
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Wafer stack&#039;&#039;&#039;&lt;br /&gt;
* Si 220 ± 10 nm&lt;br /&gt;
* BOX 3000 ± 50 nm&lt;br /&gt;
* Handle 725 ± 25 µm&lt;br /&gt;
* Cladding: air&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key numbers&#039;&#039;&#039;&lt;br /&gt;
* Loss: ~1.7–2.3 dB/cm (0.50 µm)&lt;br /&gt;
* Etch rate: ~5.9 nm/s&lt;br /&gt;
* Etch depth: 228–232 nm&lt;br /&gt;
* Si : ZEP selectivity: 1.55 : 1&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
{| class=&amp;quot;wikitable mw-collapsible mw-collapsed&amp;quot; style=&amp;quot;width:100%;&amp;quot;&lt;br /&gt;
! style=&amp;quot;text-align:left;&amp;quot; | EBL data preparation (BEAMER)&lt;br /&gt;
|-&lt;br /&gt;
|&lt;br /&gt;
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.&lt;br /&gt;
* &#039;&#039;&#039;Waveguide bias:&#039;&#039;&#039; +7 nm per edge.&lt;br /&gt;
* &#039;&#039;&#039;Sleeve (fine):&#039;&#039;&#039; 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Bulk (coarse):&#039;&#039;&#039; band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Assist:&#039;&#039;&#039; waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.&lt;br /&gt;
* &#039;&#039;&#039;Fields:&#039;&#039;&#039; 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.&lt;br /&gt;
* &#039;&#039;&#039;PEC:&#039;&#039;&#039; Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
{| class=&amp;quot;wikitable mw-collapsible mw-collapsed&amp;quot; style=&amp;quot;width:100%;&amp;quot;&lt;br /&gt;
! style=&amp;quot;text-align:left;&amp;quot; | Si etch sequence&lt;br /&gt;
|-&lt;br /&gt;
|&lt;br /&gt;
Every etch session conditions the chamber first, then runs a two-step etch.&lt;br /&gt;
# &#039;&#039;&#039;O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; chamber clean:&#039;&#039;&#039; 5 min minimum, typically 10 min.&lt;br /&gt;
# &#039;&#039;&#039;SF&amp;lt;sub&amp;gt;6&amp;lt;/sub&amp;gt;/O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; clean:&#039;&#039;&#039; 5 min.&lt;br /&gt;
# &#039;&#039;&#039;Si precondition:&#039;&#039;&#039; 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.&lt;br /&gt;
# &#039;&#039;&#039;Load sample&#039;&#039;&#039; on a carrier wafer with oil.&lt;br /&gt;
# &#039;&#039;&#039;Stabilise (strike) step:&#039;&#039;&#039; ~6 s; etches ~38 nm, so include it in the depth budget.&lt;br /&gt;
# &#039;&#039;&#039;Main etch:&#039;&#039;&#039; ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.&lt;br /&gt;
&lt;br /&gt;
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.&lt;br /&gt;
|}&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=59</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=59"/>
		<updated>2026-11-13T01:36:07Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: &lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: &#039;&#039;&#039;1.72 ± 0.21 dB/cm&#039;&#039;&#039; (0.50 µm strip, air-clad).&lt;br /&gt;
&lt;br /&gt;
[[File:SOI220_Standard_Process_Flow.png|left|1200px|220 nm SOI standard process flow]]&lt;br /&gt;
&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
| style=&amp;quot;width:70%; vertical-align:top;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate clean&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry. 5 min dehydration bake at 180 °C, then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma (200 W, 100 sccm O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt;, 10 mTorr).&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood and sonicator&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — Resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; before dispensing.&lt;br /&gt;
&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 3 — Pre-exposure bake&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe &amp;quot;ZEP520A on SOI&amp;quot;).&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
* Filmtek&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 4 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose at 100 kV as two passes from one BEAMER flow (see &#039;&#039;EBL data preparation&#039;&#039; below):&lt;br /&gt;
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step&lt;br /&gt;
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step&lt;br /&gt;
&lt;br /&gt;
* CMM — Raith EBPG5150 (100 kV)&lt;br /&gt;
* Process flow PDF: [[index.php?title=Media:SiCOI litho.pdf|SiCOI litho]]&amp;lt;!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --&amp;gt;&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 5 — Development&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 6 — Resist reflow (optional)&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 7 — Si etch&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see &#039;&#039;Si etch sequence&#039;&#039; below). Si : ZEP selectivity is ~1.55 : 1.&lt;br /&gt;
&lt;br /&gt;
* ANFF-Q — Oxford ICP-RIE&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 8 — Resist removal&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma at 200 W.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood, Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 9 — Inspection&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.&lt;br /&gt;
&lt;br /&gt;
* Optical microscope&lt;br /&gt;
* CMM — Dektak; ANFF-Q — KLA profiler&lt;br /&gt;
* CMM — eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 10 — Dicing&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Coat with AZ protective resist, dice, then solvent clean as in Step 1.&lt;br /&gt;
&lt;br /&gt;
* Sawatec spin coater (protective coat)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
| style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — clean, coat, EBL, metrology&lt;br /&gt;
* ANFF-Q (AIBN) — etch, depth profiling&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150 (100 kV EBL)&lt;br /&gt;
* BEAMER (EBL data preparation)&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
* Oxford ICP-RIE&lt;br /&gt;
* Diener plasma cleaner&lt;br /&gt;
* CEE Apogee spin coater&lt;br /&gt;
* Filmtek (film thickness)&lt;br /&gt;
* Dektak / KLA (step height)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone (standard process)&lt;br /&gt;
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Wafer stack&#039;&#039;&#039;&lt;br /&gt;
* Si 220 ± 10 nm&lt;br /&gt;
* BOX 3000 ± 50 nm&lt;br /&gt;
* Handle 725 ± 25 µm&lt;br /&gt;
* Cladding: air&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key numbers&#039;&#039;&#039;&lt;br /&gt;
* Loss: ~1.7–2.3 dB/cm (0.50 µm)&lt;br /&gt;
* Etch rate: ~5.9 nm/s&lt;br /&gt;
* Etch depth: 228–232 nm&lt;br /&gt;
* Si : ZEP selectivity: 1.55 : 1&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;EBL data preparation (BEAMER)&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.&lt;br /&gt;
* &#039;&#039;&#039;Waveguide bias:&#039;&#039;&#039; +7 nm per edge.&lt;br /&gt;
* &#039;&#039;&#039;Sleeve (fine):&#039;&#039;&#039; 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Bulk (coarse):&#039;&#039;&#039; band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Assist:&#039;&#039;&#039; waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.&lt;br /&gt;
* &#039;&#039;&#039;Fields:&#039;&#039;&#039; 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.&lt;br /&gt;
* &#039;&#039;&#039;PEC:&#039;&#039;&#039; Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Si etch sequence&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Every etch session conditions the chamber first, then runs a two-step etch.&lt;br /&gt;
# &#039;&#039;&#039;O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; chamber clean:&#039;&#039;&#039; 5 min minimum, typically 10 min.&lt;br /&gt;
# &#039;&#039;&#039;SF&amp;lt;sub&amp;gt;6&amp;lt;/sub&amp;gt;/O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; clean:&#039;&#039;&#039; 5 min.&lt;br /&gt;
# &#039;&#039;&#039;Si precondition:&#039;&#039;&#039; 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.&lt;br /&gt;
# &#039;&#039;&#039;Load sample&#039;&#039;&#039; on a carrier wafer with oil.&lt;br /&gt;
# &#039;&#039;&#039;Stabilise (strike) step:&#039;&#039;&#039; ~6 s; etches ~38 nm, so include it in the depth budget.&lt;br /&gt;
# &#039;&#039;&#039;Main etch:&#039;&#039;&#039; ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.&lt;br /&gt;
&lt;br /&gt;
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Process flow website&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Interactive version of this process flow: [http://SERVER/photonics.html Photonics process flow] &amp;lt;!-- replace SERVER with the hosting machine&#039;s name; localhost only works on that machine --&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=57</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=57"/>
		<updated>2026-11-13T01:35:21Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: &lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: &#039;&#039;&#039;1.72 ± 0.21 dB/cm&#039;&#039;&#039; (0.50 µm strip, air-clad).&lt;br /&gt;
&lt;br /&gt;
[[File:SOI220_Standard_Process_Flow.png|center|1000px|220 nm SOI standard process flow]]&lt;br /&gt;
&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
| style=&amp;quot;width:70%; vertical-align:top;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate clean&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry. 5 min dehydration bake at 180 °C, then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma (200 W, 100 sccm O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt;, 10 mTorr).&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood and sonicator&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — Resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; before dispensing.&lt;br /&gt;
&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 3 — Pre-exposure bake&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe &amp;quot;ZEP520A on SOI&amp;quot;).&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
* Filmtek&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 4 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose at 100 kV as two passes from one BEAMER flow (see &#039;&#039;EBL data preparation&#039;&#039; below):&lt;br /&gt;
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step&lt;br /&gt;
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step&lt;br /&gt;
&lt;br /&gt;
* CMM — Raith EBPG5150 (100 kV)&lt;br /&gt;
* Process flow PDF: [[index.php?title=Media:SiCOI litho.pdf|SiCOI litho]]&amp;lt;!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --&amp;gt;&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 5 — Development&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 6 — Resist reflow (optional)&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 7 — Si etch&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see &#039;&#039;Si etch sequence&#039;&#039; below). Si : ZEP selectivity is ~1.55 : 1.&lt;br /&gt;
&lt;br /&gt;
* ANFF-Q — Oxford ICP-RIE&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 8 — Resist removal&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma at 200 W.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood, Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 9 — Inspection&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.&lt;br /&gt;
&lt;br /&gt;
* Optical microscope&lt;br /&gt;
* CMM — Dektak; ANFF-Q — KLA profiler&lt;br /&gt;
* CMM — eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 10 — Dicing&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Coat with AZ protective resist, dice, then solvent clean as in Step 1.&lt;br /&gt;
&lt;br /&gt;
* Sawatec spin coater (protective coat)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
| style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — clean, coat, EBL, metrology&lt;br /&gt;
* ANFF-Q (AIBN) — etch, depth profiling&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150 (100 kV EBL)&lt;br /&gt;
* BEAMER (EBL data preparation)&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
* Oxford ICP-RIE&lt;br /&gt;
* Diener plasma cleaner&lt;br /&gt;
* CEE Apogee spin coater&lt;br /&gt;
* Filmtek (film thickness)&lt;br /&gt;
* Dektak / KLA (step height)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone (standard process)&lt;br /&gt;
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Wafer stack&#039;&#039;&#039;&lt;br /&gt;
* Si 220 ± 10 nm&lt;br /&gt;
* BOX 3000 ± 50 nm&lt;br /&gt;
* Handle 725 ± 25 µm&lt;br /&gt;
* Cladding: air&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key numbers&#039;&#039;&#039;&lt;br /&gt;
* Loss: ~1.7–2.3 dB/cm (0.50 µm)&lt;br /&gt;
* Etch rate: ~5.9 nm/s&lt;br /&gt;
* Etch depth: 228–232 nm&lt;br /&gt;
* Si : ZEP selectivity: 1.55 : 1&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;EBL data preparation (BEAMER)&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.&lt;br /&gt;
* &#039;&#039;&#039;Waveguide bias:&#039;&#039;&#039; +7 nm per edge.&lt;br /&gt;
* &#039;&#039;&#039;Sleeve (fine):&#039;&#039;&#039; 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Bulk (coarse):&#039;&#039;&#039; band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Assist:&#039;&#039;&#039; waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.&lt;br /&gt;
* &#039;&#039;&#039;Fields:&#039;&#039;&#039; 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.&lt;br /&gt;
* &#039;&#039;&#039;PEC:&#039;&#039;&#039; Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Si etch sequence&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Every etch session conditions the chamber first, then runs a two-step etch.&lt;br /&gt;
# &#039;&#039;&#039;O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; chamber clean:&#039;&#039;&#039; 5 min minimum, typically 10 min.&lt;br /&gt;
# &#039;&#039;&#039;SF&amp;lt;sub&amp;gt;6&amp;lt;/sub&amp;gt;/O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; clean:&#039;&#039;&#039; 5 min.&lt;br /&gt;
# &#039;&#039;&#039;Si precondition:&#039;&#039;&#039; 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.&lt;br /&gt;
# &#039;&#039;&#039;Load sample&#039;&#039;&#039; on a carrier wafer with oil.&lt;br /&gt;
# &#039;&#039;&#039;Stabilise (strike) step:&#039;&#039;&#039; ~6 s; etches ~38 nm, so include it in the depth budget.&lt;br /&gt;
# &#039;&#039;&#039;Main etch:&#039;&#039;&#039; ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.&lt;br /&gt;
&lt;br /&gt;
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Process flow website&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Interactive version of this process flow: [http://SERVER/photonics.html Photonics process flow] &amp;lt;!-- replace SERVER with the hosting machine&#039;s name; localhost only works on that machine --&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=55</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=55"/>
		<updated>2026-11-13T01:34:57Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: Added basic SOI process flow image.&lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: &#039;&#039;&#039;1.72 ± 0.21 dB/cm&#039;&#039;&#039; (0.50 µm strip, air-clad).&lt;br /&gt;
&lt;br /&gt;
[[File:SOI220 Standard Process Flow.png|thumb|975x975px|SOI220 Standard Process Flow]]&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
| style=&amp;quot;width:70%; vertical-align:top;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate clean&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry. 5 min dehydration bake at 180 °C, then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma (200 W, 100 sccm O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt;, 10 mTorr).&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood and sonicator&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — Resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; before dispensing.&lt;br /&gt;
&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 3 — Pre-exposure bake&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe &amp;quot;ZEP520A on SOI&amp;quot;).&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
* Filmtek&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 4 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose at 100 kV as two passes from one BEAMER flow (see &#039;&#039;EBL data preparation&#039;&#039; below):&lt;br /&gt;
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step&lt;br /&gt;
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step&lt;br /&gt;
&lt;br /&gt;
* CMM — Raith EBPG5150 (100 kV)&lt;br /&gt;
* Process flow PDF: [[index.php?title=Media:SiCOI litho.pdf|SiCOI litho]]&amp;lt;!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --&amp;gt;&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 5 — Development&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 6 — Resist reflow (optional)&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 7 — Si etch&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see &#039;&#039;Si etch sequence&#039;&#039; below). Si : ZEP selectivity is ~1.55 : 1.&lt;br /&gt;
&lt;br /&gt;
* ANFF-Q — Oxford ICP-RIE&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 8 — Resist removal&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma at 200 W.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood, Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 9 — Inspection&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.&lt;br /&gt;
&lt;br /&gt;
* Optical microscope&lt;br /&gt;
* CMM — Dektak; ANFF-Q — KLA profiler&lt;br /&gt;
* CMM — eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 10 — Dicing&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Coat with AZ protective resist, dice, then solvent clean as in Step 1.&lt;br /&gt;
&lt;br /&gt;
* Sawatec spin coater (protective coat)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
| style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot; |&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — clean, coat, EBL, metrology&lt;br /&gt;
* ANFF-Q (AIBN) — etch, depth profiling&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150 (100 kV EBL)&lt;br /&gt;
* BEAMER (EBL data preparation)&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
* Oxford ICP-RIE&lt;br /&gt;
* Diener plasma cleaner&lt;br /&gt;
* CEE Apogee spin coater&lt;br /&gt;
* Filmtek (film thickness)&lt;br /&gt;
* Dektak / KLA (step height)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone (standard process)&lt;br /&gt;
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Wafer stack&#039;&#039;&#039;&lt;br /&gt;
* Si 220 ± 10 nm&lt;br /&gt;
* BOX 3000 ± 50 nm&lt;br /&gt;
* Handle 725 ± 25 µm&lt;br /&gt;
* Cladding: air&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key numbers&#039;&#039;&#039;&lt;br /&gt;
* Loss: ~1.7–2.3 dB/cm (0.50 µm)&lt;br /&gt;
* Etch rate: ~5.9 nm/s&lt;br /&gt;
* Etch depth: 228–232 nm&lt;br /&gt;
* Si : ZEP selectivity: 1.55 : 1&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;EBL data preparation (BEAMER)&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.&lt;br /&gt;
* &#039;&#039;&#039;Waveguide bias:&#039;&#039;&#039; +7 nm per edge.&lt;br /&gt;
* &#039;&#039;&#039;Sleeve (fine):&#039;&#039;&#039; 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Bulk (coarse):&#039;&#039;&#039; band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Assist:&#039;&#039;&#039; waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.&lt;br /&gt;
* &#039;&#039;&#039;Fields:&#039;&#039;&#039; 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.&lt;br /&gt;
* &#039;&#039;&#039;PEC:&#039;&#039;&#039; Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Si etch sequence&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Every etch session conditions the chamber first, then runs a two-step etch.&lt;br /&gt;
# &#039;&#039;&#039;O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; chamber clean:&#039;&#039;&#039; 5 min minimum, typically 10 min.&lt;br /&gt;
# &#039;&#039;&#039;SF&amp;lt;sub&amp;gt;6&amp;lt;/sub&amp;gt;/O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; clean:&#039;&#039;&#039; 5 min.&lt;br /&gt;
# &#039;&#039;&#039;Si precondition:&#039;&#039;&#039; 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.&lt;br /&gt;
# &#039;&#039;&#039;Load sample&#039;&#039;&#039; on a carrier wafer with oil.&lt;br /&gt;
# &#039;&#039;&#039;Stabilise (strike) step:&#039;&#039;&#039; ~6 s; etches ~38 nm, so include it in the depth budget.&lt;br /&gt;
# &#039;&#039;&#039;Main etch:&#039;&#039;&#039; ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.&lt;br /&gt;
&lt;br /&gt;
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Process flow website&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Interactive version of this process flow: [http://SERVER/photonics.html Photonics process flow] &amp;lt;!-- replace SERVER with the hosting machine&#039;s name; localhost only works on that machine --&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=File:SOI220_Standard_Process_Flow.png&amp;diff=53</id>
		<title>File:SOI220 Standard Process Flow.png</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=File:SOI220_Standard_Process_Flow.png&amp;diff=53"/>
		<updated>2026-11-13T01:33:47Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: &lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;SOI220 Standard Process Flow&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=51</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=51"/>
		<updated>2026-11-13T01:11:02Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: /* Basic information and section added for 220nm SOI photonics to Photonics — Si photonics, metalenses, integrated photonics */&lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: &#039;&#039;&#039;1.72 ± 0.21 dB/cm&#039;&#039;&#039; (0.50 µm strip, air-clad).&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Clean → Spin coat → Bake → EBL exposure → Develop → (Reflow) → Si etch → Resist strip → Inspect → Dice&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
|style=&amp;quot;width:70%; vertical-align:top;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate clean&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry. 5 min dehydration bake at 180 °C, then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma (200 W, 100 sccm O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt;, 10 mTorr).&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood and sonicator&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — Resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; before dispensing.&lt;br /&gt;
&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 3 — Pre-exposure bake&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe &amp;quot;ZEP520A on SOI&amp;quot;).&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
* Filmtek&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 4 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose at 100 kV as two passes from one BEAMER flow (see &#039;&#039;EBL data preparation&#039;&#039; below):&lt;br /&gt;
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step&lt;br /&gt;
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step&lt;br /&gt;
&lt;br /&gt;
* CMM — Raith EBPG5150 (100 kV)&lt;br /&gt;
* Process flow PDF: [[Media:SiCOI litho.pdf|SiCOI litho]] &amp;lt;!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --&amp;gt;&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 5 — Development&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; dry.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 6 — Resist reflow (optional)&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.&lt;br /&gt;
&lt;br /&gt;
* Hotplate&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 7 — Si etch&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see &#039;&#039;Si etch sequence&#039;&#039; below). Si : ZEP selectivity is ~1.55 : 1.&lt;br /&gt;
&lt;br /&gt;
* ANFF-Q — Oxford ICP-RIE&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 8 — Resist removal&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; plasma at 200 W.&lt;br /&gt;
&lt;br /&gt;
* CMM — fume hood, Diener plasma cleaner&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 9 — Inspection&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.&lt;br /&gt;
&lt;br /&gt;
* Optical microscope&lt;br /&gt;
* CMM — Dektak; ANFF-Q — KLA profiler&lt;br /&gt;
* CMM — eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 10 — Dicing&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Coat with AZ protective resist, dice, then solvent clean as in Step 1.&lt;br /&gt;
&lt;br /&gt;
* Sawatec spin coater (protective coat)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
|style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — clean, coat, EBL, metrology&lt;br /&gt;
* ANFF-Q (AIBN) — etch, depth profiling&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150 (100 kV EBL)&lt;br /&gt;
* BEAMER (EBL data preparation)&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
* Oxford ICP-RIE&lt;br /&gt;
* Diener plasma cleaner&lt;br /&gt;
* CEE Apogee spin coater&lt;br /&gt;
* Filmtek (film thickness)&lt;br /&gt;
* Dektak / KLA (step height)&lt;br /&gt;
* Accretech dicing saw&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone (standard process)&lt;br /&gt;
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Wafer stack&#039;&#039;&#039;&lt;br /&gt;
* Si 220 ± 10 nm&lt;br /&gt;
* BOX 3000 ± 50 nm&lt;br /&gt;
* Handle 725 ± 25 µm&lt;br /&gt;
* Cladding: air&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key numbers&#039;&#039;&#039;&lt;br /&gt;
* Loss: ~1.7–2.3 dB/cm (0.50 µm)&lt;br /&gt;
* Etch rate: ~5.9 nm/s&lt;br /&gt;
* Etch depth: 228–232 nm&lt;br /&gt;
* Si : ZEP selectivity: 1.55 : 1&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;EBL data preparation (BEAMER)&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.&lt;br /&gt;
* &#039;&#039;&#039;Waveguide bias:&#039;&#039;&#039; +7 nm per edge.&lt;br /&gt;
* &#039;&#039;&#039;Sleeve (fine):&#039;&#039;&#039; 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Bulk (coarse):&#039;&#039;&#039; band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.&lt;br /&gt;
* &#039;&#039;&#039;Assist:&#039;&#039;&#039; waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.&lt;br /&gt;
* &#039;&#039;&#039;Fields:&#039;&#039;&#039; 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.&lt;br /&gt;
* &#039;&#039;&#039;PEC:&#039;&#039;&#039; Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Si etch sequence&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Every etch session conditions the chamber first, then runs a two-step etch.&lt;br /&gt;
# &#039;&#039;&#039;O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; chamber clean:&#039;&#039;&#039; 5 min minimum, typically 10 min.&lt;br /&gt;
# &#039;&#039;&#039;SF&amp;lt;sub&amp;gt;6&amp;lt;/sub&amp;gt;/O&amp;lt;sub&amp;gt;2&amp;lt;/sub&amp;gt; clean:&#039;&#039;&#039; 5 min.&lt;br /&gt;
# &#039;&#039;&#039;Si precondition:&#039;&#039;&#039; 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.&lt;br /&gt;
# &#039;&#039;&#039;Load sample&#039;&#039;&#039; on a carrier wafer with oil.&lt;br /&gt;
# &#039;&#039;&#039;Stabilise (strike) step:&#039;&#039;&#039; ~6 s; etches ~38 nm, so include it in the depth budget.&lt;br /&gt;
# &#039;&#039;&#039;Main etch:&#039;&#039;&#039; ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.&lt;br /&gt;
&lt;br /&gt;
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Process flow website&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
Interactive version of this process flow: [http://SERVER/photonics.html Photonics process flow] &amp;lt;!-- replace SERVER with the hosting machine&#039;s name; localhost only works on that machine --&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
	<entry>
		<id>https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=49</id>
		<title>Photonics</title>
		<link rel="alternate" type="text/html" href="https://wiki.cmm.uq.edu.au/index.php?title=Photonics&amp;diff=49"/>
		<updated>2026-11-13T00:56:08Z</updated>

		<summary type="html">&lt;p&gt;UQdpeace: /* Daniel edit test. Photonics — Si photonics, metalenses, integrated photonics */&lt;/p&gt;
&lt;hr /&gt;
&lt;div&gt;== Photonics — Si photonics, metalenses, integrated photonics ==&lt;br /&gt;
&#039;&#039;Nanofabrication workflows for integrated photonic devices.&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===&lt;br /&gt;
Updated: 13/11/2026&lt;br /&gt;
&lt;br /&gt;
==== Silicon photonics — waveguides, ring resonators, grating couplers ====&lt;br /&gt;
EBL-defined silicon-on-insulator (SOI) waveguide devices. Critical dimensions typically 200–500 nm width.&lt;br /&gt;
&lt;br /&gt;
{| style=&amp;quot;width:100%;&amp;quot; cellpadding=&amp;quot;10&amp;quot; valign=&amp;quot;top&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
|style=&amp;quot;width:70%; vertical-align:top;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Step 1 — Substrate prep and resist coating&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Clean SOI wafer in plasma cleaner. Spin ZEP520A or HSQ 6%.&lt;br /&gt;
&lt;br /&gt;
* CMM — Diener plasma cleaner&lt;br /&gt;
* CMM — CEE Apogee spin coater&lt;br /&gt;
&lt;br /&gt;
----&lt;br /&gt;
&#039;&#039;&#039;Step 2 — EBL exposure&#039;&#039;&#039;&lt;br /&gt;
&lt;br /&gt;
Expose waveguide layout at 100 kV. Typical dose: 160–200 µC/cm².&lt;br /&gt;
&lt;br /&gt;
* EBPG5150 (100 kV)&lt;br /&gt;
** Adding a pdf process flow [[index.php?title=Media:SiCOI litho.pdf|SiCOI litho]]&lt;br /&gt;
* eLINE Plus (CD-SEM)&lt;br /&gt;
&lt;br /&gt;
|style=&amp;quot;width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;&amp;quot;|&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Facilities used&#039;&#039;&#039;&lt;br /&gt;
* CMM (Hawken) — EBL + metro&lt;br /&gt;
* ANFF-Q (AIBN) — etch / dep.&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Key instruments&#039;&#039;&#039;&lt;br /&gt;
* Raith EBPG5150&lt;br /&gt;
* eLINE Plus&lt;br /&gt;
* Oxford RIE / Prog 200&lt;br /&gt;
&lt;br /&gt;
&#039;&#039;&#039;Typical resists&#039;&#039;&#039;&lt;br /&gt;
* ZEP520A — positive tone&lt;br /&gt;
* HSQ 6% — negative tone hard mask&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible mw-collapsed&amp;quot;&amp;gt;&lt;br /&gt;
&#039;&#039;&#039;Collapsable html website&#039;&#039;&#039;&lt;br /&gt;
&amp;lt;div class=&amp;quot;mw-collapsible-content&amp;quot;&amp;gt;&lt;br /&gt;
We can add a html to the MediaWiki format if we want. Or we can just add a link.&lt;br /&gt;
&lt;br /&gt;
* Link &amp;lt;iframe src=&amp;quot;http://localhost/photonics.html&amp;quot; width=&amp;quot;100%&amp;quot; height=&amp;quot;800px&amp;quot; frameborder=&amp;quot;0&amp;quot;&amp;gt;&amp;lt;/iframe&amp;gt;&lt;br /&gt;
&lt;br /&gt;
* Embbedded html&lt;br /&gt;
&amp;lt;html&amp;gt;&lt;br /&gt;
&amp;lt;iframe src=&amp;quot;http://localhost/photonics.html&amp;quot; width=&amp;quot;100%&amp;quot; height=&amp;quot;800px&amp;quot; frameborder=&amp;quot;0&amp;quot;&amp;gt;&amp;lt;/iframe&amp;gt;&lt;br /&gt;
&amp;lt;/html&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;br /&gt;
&amp;lt;/div&amp;gt;&lt;/div&gt;</summary>
		<author><name>UQdpeace</name></author>
	</entry>
</feed>