Photonics: Difference between revisions

From CMM Wiki
Jump to navigationJump to search
Created page with "== Photonics — Si photonics, metalenses, integrated photonics == ''Nanofabrication workflows for integrated photonic devices.'' === Si Photonics (waveguides, rings) === ==== Silicon photonics — waveguides, ring resonators, grating couplers ==== EBL-defined silicon-on-insulator (SOI) waveguide devices. Critical dimensions typically 200–500 nm width. {| style="width:100%;" cellpadding="10" valign="top" |- |style="width:70%; vertical-align:top;"| '''Step 1 — Sub..."
 
 
(7 intermediate revisions by 2 users not shown)
Line 1: Line 1:
== Photonics — Si photonics, metalenses, integrated photonics ==
== Photonics — Si photonics, metalenses, integrated photonics ==
''Nanofabrication workflows for integrated photonic devices.''
''Nanofabrication workflows for integrated photonic devices. For each of the steps, you can check the tool type and specifications: Dicing saw (link to ANFF dicing saw); Spincoater (link to Sawatec ANFF, link to CMM spincoater); EBPG (Link to Raith ebpg CMM); Etching (Link to RIE and ICP - ANFF); Deposition (Link to e-beam evaporator and Sputterer ANFF) -> Make it bullet points (expandable window)''
[[File:Photonic circuit process flow v2.png|none|left|Typical process flow of a photonic integrated circuit]]


=== Si Photonics (waveguides, rings) ===
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===
Updated: 13/11/2026


==== Silicon photonics — waveguides, ring resonators, grating couplers ====
==== Silicon photonics — waveguides, ring resonators, grating couplers ====
EBL-defined silicon-on-insulator (SOI) waveguide devices. Critical dimensions typically 200–500 nm width.
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: '''1.72 ± 0.21 dB/cm''' (0.50 µm strip, air-clad).
 
[[File:SOI220_Standard_Process_Flow.png|left|1200px|220 nm SOI standard process flow]]


{| style="width:100%;" cellpadding="10" valign="top"
{| style="width:100%;" cellpadding="10" valign="top"
Line 11: Line 15:
|style="width:70%; vertical-align:top;"|
|style="width:70%; vertical-align:top;"|


'''Step 1 — Substrate prep and resist coating'''
'''Step 1 — Substrate clean'''


Clean SOI wafer in plasma cleaner. Spin ZEP520A or HSQ 6%.
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N<sub>2</sub> dry. 5 min dehydration bake at 180 °C, then 5 min O<sub>2</sub> plasma (200 W, 100 sccm O<sub>2</sub>, 10 mTorr).


* CMM — fume hood and sonicator
* CMM — Diener plasma cleaner
* CMM — Diener plasma cleaner
----
'''Step 2 — Resist coating'''
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N<sub>2</sub> before dispensing.
* CMM — CEE Apogee spin coater
* CMM — CEE Apogee spin coater


----
----
'''Step 2 — EBL exposure'''
'''Step 3 — Pre-exposure bake'''


Expose waveguide layout at 100 kV. Typical dose: 160–200 µC/cm².
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI").


* EBPG5150 (100 kV)
* Hotplate
** Adding a pdf process flow [[Media:SiCOI litho.pdf|SiCOI litho]]
* Filmtek
* eLINE Plus (CD-SEM)
 
----
'''Step 4 — EBL exposure'''
 
Expose at 100 kV as two passes from one BEAMER flow (see ''EBL data preparation'' below):
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step
 
* CMM — Raith EBPG5150 (100 kV)
* Process flow PDF: [[index.php?title=Media:SiCOI litho.pdf|SiCOI litho]]<!-- check: this is the SiC-on-insulator flow, not 220 nm SOI -->
 
----
'''Step 5 — Development'''
 
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N<sub>2</sub> dry.
 
* CMM — fume hood
 
----
'''Step 6 — Resist reflow (optional)'''
 
135–140 °C for 60–120 s, to smooth the resist sidewall before etching.
 
* Hotplate
 
----
'''Step 7 — Si etch'''
 
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see ''Si etch sequence'' below). Si : ZEP selectivity is ~1.55 : 1.
 
* ANFF-Q — Oxford ICP-RIE
 
----
'''Step 8 — Resist removal'''
 
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O<sub>2</sub> plasma at 200 W.
 
* CMM — fume hood, Diener plasma cleaner
 
----
'''Step 9 — Inspection'''
 
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.
 
* Optical microscope
* CMM — Dektak; ANFF-Q — KLA profiler
* CMM — eLINE Plus (CD-SEM)
 
----
'''Step 10 — Dicing'''
 
Coat with AZ protective resist, dice, then solvent clean as in Step 1.
 
* Sawatec spin coater (protective coat)
* Accretech dicing saw


|style="width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;"|
|style="width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;"|


'''Facilities used'''
'''Facilities used'''
* CMM (Hawken) — EBL + metro
* CMM (Hawken) — clean, coat, EBL, metrology
* ANFF-Q (AIBN) — etch / dep.
* ANFF-Q (AIBN) — etch, depth profiling


'''Key instruments'''
'''Key instruments'''
* Raith EBPG5150
* Raith EBPG5150 (100 kV EBL)
* eLINE Plus
* BEAMER (EBL data preparation)
* Oxford RIE / Prog 200
* eLINE Plus (CD-SEM)
* Oxford ICP-RIE
* Diener plasma cleaner
* CEE Apogee spin coater
* Filmtek (film thickness)
* Dektak / KLA (step height)
* Accretech dicing saw


'''Typical resists'''
'''Typical resists'''
* ZEP520A — positive tone
* ZEP520A — positive tone (standard process)
* HSQ 6% — negative tone hard mask
* HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)
|}


'''Wafer stack'''
* Si 220 ± 10 nm
* BOX 3000 ± 50 nm
* Handle 725 ± 25 µm
* Cladding: air


'''Key numbers'''
* Loss: ~1.7–2.3 dB/cm (0.50 µm)
* Etch rate: ~5.9 nm/s
* Etch depth: 228–232 nm
* Si : ZEP selectivity: 1.55 : 1
|}


<div class="mw-collapsible mw-collapsed">
{| class="wikitable mw-collapsible mw-collapsed" style="width:100%;"
'''Collapsable html website'''
! style="text-align:left;" | EBL data preparation (BEAMER)
<div class="mw-collapsible-content">
|-
We can add a html to the MediaWiki format if we want. Or we can just add a link.
|
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.
* '''Waveguide bias:''' +7 nm per edge.
* '''Sleeve (fine):''' 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.
* '''Bulk (coarse):''' band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.
* '''Assist:''' waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.
* '''Fields:''' 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.
* '''PEC:''' Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).
|}


* Link <iframe src="http://localhost/photonics.html" width="100%" height="800px" frameborder="0"></iframe>
{| class="wikitable mw-collapsible mw-collapsed" style="width:100%;"
! style="text-align:left;" | Si etch sequence
|-
|
Every etch session conditions the chamber first, then runs a two-step etch.
# '''O<sub>2</sub> chamber clean:''' 5 min minimum, typically 10 min.
# '''SF<sub>6</sub>/O<sub>2</sub> clean:''' 5 min.
# '''Si precondition:''' 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.
# '''Load sample''' on a carrier wafer with oil.
# '''Stabilise (strike) step:''' ~6 s; etches ~38 nm, so include it in the depth budget.
# '''Main etch:''' ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.


* Embbedded html
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.
<html>
|}
<iframe src="http://localhost/photonics.html" width="100%" height="800px" frameborder="0"></iframe>
</html>
</div>
</div>

Latest revision as of 13:03, 17 November 2026

Photonics — Si photonics, metalenses, integrated photonics

Nanofabrication workflows for integrated photonic devices. For each of the steps, you can check the tool type and specifications: Dicing saw (link to ANFF dicing saw); Spincoater (link to Sawatec ANFF, link to CMM spincoater); EBPG (Link to Raith ebpg CMM); Etching (Link to RIE and ICP - ANFF); Deposition (Link to e-beam evaporator and Sputterer ANFF) -> Make it bullet points (expandable window)

Typical process flow of a photonic integrated circuit
Typical process flow of a photonic integrated circuit

220nm Silicon-on-Insulator Photonics - Standard Process

Updated: 13/11/2026

Silicon photonics — waveguides, ring resonators, grating couplers

EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: 1.72 ± 0.21 dB/cm (0.50 µm strip, air-clad).

220 nm SOI standard process flow
220 nm SOI standard process flow

Step 1 — Substrate clean

10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N2 dry. 5 min dehydration bake at 180 °C, then 5 min O2 plasma (200 W, 100 sccm O2, 10 mTorr).

  • CMM — fume hood and sonicator
  • CMM — Diener plasma cleaner

Step 2 — Resist coating

Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N2 before dispensing.

  • CMM — CEE Apogee spin coater

Step 3 — Pre-exposure bake

180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI").

  • Hotplate
  • Filmtek

Step 4 — EBL exposure

Expose at 100 kV as two passes from one BEAMER flow (see EBL data preparation below):

  • Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step
  • Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step
  • CMM — Raith EBPG5150 (100 kV)
  • Process flow PDF: SiCOI litho

Step 5 — Development

60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N2 dry.

  • CMM — fume hood

Step 6 — Resist reflow (optional)

135–140 °C for 60–120 s, to smooth the resist sidewall before etching.

  • Hotplate

Step 7 — Si etch

Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see Si etch sequence below). Si : ZEP selectivity is ~1.55 : 1.

  • ANFF-Q — Oxford ICP-RIE

Step 8 — Resist removal

Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O2 plasma at 200 W.

  • CMM — fume hood, Diener plasma cleaner

Step 9 — Inspection

Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.

  • Optical microscope
  • CMM — Dektak; ANFF-Q — KLA profiler
  • CMM — eLINE Plus (CD-SEM)

Step 10 — Dicing

Coat with AZ protective resist, dice, then solvent clean as in Step 1.

  • Sawatec spin coater (protective coat)
  • Accretech dicing saw

Facilities used

  • CMM (Hawken) — clean, coat, EBL, metrology
  • ANFF-Q (AIBN) — etch, depth profiling

Key instruments

  • Raith EBPG5150 (100 kV EBL)
  • BEAMER (EBL data preparation)
  • eLINE Plus (CD-SEM)
  • Oxford ICP-RIE
  • Diener plasma cleaner
  • CEE Apogee spin coater
  • Filmtek (film thickness)
  • Dektak / KLA (step height)
  • Accretech dicing saw

Typical resists

  • ZEP520A — positive tone (standard process)
  • HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)

Wafer stack

  • Si 220 ± 10 nm
  • BOX 3000 ± 50 nm
  • Handle 725 ± 25 µm
  • Cladding: air

Key numbers

  • Loss: ~1.7–2.3 dB/cm (0.50 µm)
  • Etch rate: ~5.9 nm/s
  • Etch depth: 228–232 nm
  • Si : ZEP selectivity: 1.55 : 1
EBL data preparation (BEAMER)

Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.

  • Waveguide bias: +7 nm per edge.
  • Sleeve (fine): 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.
  • Bulk (coarse): band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.
  • Assist: waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.
  • Fields: 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.
  • PEC: Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).
Si etch sequence

Every etch session conditions the chamber first, then runs a two-step etch.

  1. O2 chamber clean: 5 min minimum, typically 10 min.
  2. SF6/O2 clean: 5 min.
  3. Si precondition: 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.
  4. Load sample on a carrier wafer with oil.
  5. Stabilise (strike) step: ~6 s; etches ~38 nm, so include it in the depth budget.
  6. Main etch: ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.

Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.