Photonics: Difference between revisions
| Line 6: | Line 6: | ||
==== Silicon photonics — waveguides, ring resonators, grating couplers ==== | ==== Silicon photonics — waveguides, ring resonators, grating couplers ==== | ||
EBL-defined silicon-on-insulator (SOI) | EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: '''1.72 ± 0.21 dB/cm''' (0.50 µm strip, air-clad). | ||
'''Clean → Spin coat → Bake → EBL exposure → Develop → (Reflow) → Si etch → Resist strip → Inspect → Dice''' | |||
{| style="width:100%;" cellpadding="10" valign="top" | {| style="width:100%;" cellpadding="10" valign="top" | ||
| Line 12: | Line 14: | ||
|style="width:70%; vertical-align:top;"| | |style="width:70%; vertical-align:top;"| | ||
'''Step 1 — Substrate | '''Step 1 — Substrate clean''' | ||
10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N<sub>2</sub> dry. 5 min dehydration bake at 180 °C, then 5 min O<sub>2</sub> plasma (200 W, 100 sccm O<sub>2</sub>, 10 mTorr). | |||
* CMM — fume hood and sonicator | |||
* CMM — Diener plasma cleaner | * CMM — Diener plasma cleaner | ||
---- | |||
'''Step 2 — Resist coating''' | |||
Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N<sub>2</sub> before dispensing. | |||
* CMM — CEE Apogee spin coater | * CMM — CEE Apogee spin coater | ||
---- | ---- | ||
'''Step | '''Step 3 — Pre-exposure bake''' | ||
180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI"). | |||
* Hotplate | |||
* Filmtek | |||
---- | |||
'''Step 4 — EBL exposure''' | |||
Expose at 100 kV as two passes from one BEAMER flow (see ''EBL data preparation'' below): | |||
* Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step | |||
* Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step | |||
* CMM — Raith EBPG5150 (100 kV) | |||
* Process flow PDF: [[Media:SiCOI litho.pdf|SiCOI litho]] <!-- check: this is the SiC-on-insulator flow, not 220 nm SOI --> | |||
---- | |||
'''Step 5 — Development''' | |||
60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N<sub>2</sub> dry. | |||
* CMM — fume hood | |||
---- | |||
'''Step 6 — Resist reflow (optional)''' | |||
135–140 °C for 60–120 s, to smooth the resist sidewall before etching. | |||
* Hotplate | |||
---- | |||
'''Step 7 — Si etch''' | |||
Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see ''Si etch sequence'' below). Si : ZEP selectivity is ~1.55 : 1. | |||
* ANFF-Q — Oxford ICP-RIE | |||
---- | |||
'''Step 8 — Resist removal''' | |||
Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O<sub>2</sub> plasma at 200 W. | |||
* | * CMM — fume hood, Diener plasma cleaner | ||
** | |||
* eLINE Plus (CD-SEM) | ---- | ||
'''Step 9 — Inspection''' | |||
Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features. | |||
* Optical microscope | |||
* CMM — Dektak; ANFF-Q — KLA profiler | |||
* CMM — eLINE Plus (CD-SEM) | |||
---- | |||
'''Step 10 — Dicing''' | |||
Coat with AZ protective resist, dice, then solvent clean as in Step 1. | |||
* Sawatec spin coater (protective coat) | |||
* Accretech dicing saw | |||
|style="width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;"| | |style="width:30%; vertical-align:top; background-color:#f5f5f5; padding:10px;"| | ||
'''Facilities used''' | '''Facilities used''' | ||
* CMM (Hawken) — EBL | * CMM (Hawken) — clean, coat, EBL, metrology | ||
* ANFF-Q (AIBN) — etch | * ANFF-Q (AIBN) — etch, depth profiling | ||
'''Key instruments''' | '''Key instruments''' | ||
* Raith EBPG5150 | * Raith EBPG5150 (100 kV EBL) | ||
* eLINE Plus | * BEAMER (EBL data preparation) | ||
* Oxford RIE / | * eLINE Plus (CD-SEM) | ||
* Oxford ICP-RIE | |||
* Diener plasma cleaner | |||
* CEE Apogee spin coater | |||
* Filmtek (film thickness) | |||
* Dektak / KLA (step height) | |||
* Accretech dicing saw | |||
'''Typical resists''' | '''Typical resists''' | ||
* ZEP520A — positive tone | * ZEP520A — positive tone (standard process) | ||
* HSQ 6% — negative tone hard mask | * HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process) | ||
'''Wafer stack''' | |||
* Si 220 ± 10 nm | |||
* BOX 3000 ± 50 nm | |||
* Handle 725 ± 25 µm | |||
* Cladding: air | |||
'''Key numbers''' | |||
* Loss: ~1.7–2.3 dB/cm (0.50 µm) | |||
* Etch rate: ~5.9 nm/s | |||
* Etch depth: 228–232 nm | |||
* Si : ZEP selectivity: 1.55 : 1 | |||
|} | |} | ||
<div class="mw-collapsible mw-collapsed"> | |||
'''EBL data preparation (BEAMER)''' | |||
<div class="mw-collapsible-content"> | |||
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench. | |||
* '''Waveguide bias:''' +7 nm per edge. | |||
* '''Sleeve (fine):''' 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling. | |||
* '''Bulk (coarse):''' band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling. | |||
* '''Assist:''' waveguide + 5 µm; used only to place write fields along the waveguides, never exposed. | |||
* '''Fields:''' 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing. | |||
* '''PEC:''' Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6). | |||
</div> | |||
</div> | |||
<div class="mw-collapsible mw-collapsed"> | <div class="mw-collapsible mw-collapsed"> | ||
''' | '''Si etch sequence''' | ||
<div class="mw-collapsible-content"> | <div class="mw-collapsible-content"> | ||
Every etch session conditions the chamber first, then runs a two-step etch. | |||
# '''O<sub>2</sub> chamber clean:''' 5 min minimum, typically 10 min. | |||
# '''SF<sub>6</sub>/O<sub>2</sub> clean:''' 5 min. | |||
# '''Si precondition:''' 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading. | |||
# '''Load sample''' on a carrier wafer with oil. | |||
# '''Stabilise (strike) step:''' ~6 s; etches ~38 nm, so include it in the depth budget. | |||
# '''Main etch:''' ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch. | |||
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded. | |||
</div> | |||
</div> | |||
<div class="mw-collapsible mw-collapsed"> | |||
< | '''Process flow website''' | ||
< | <div class="mw-collapsible-content"> | ||
Interactive version of this process flow: [http://SERVER/photonics.html Photonics process flow] <!-- replace SERVER with the hosting machine's name; localhost only works on that machine --> | |||
</div> | </div> | ||
</div> | </div> | ||
Revision as of 11:11, 13 November 2026
Photonics — Si photonics, metalenses, integrated photonics
Nanofabrication workflows for integrated photonic devices.
220nm Silicon-on-Insulator Photonics - Standard Process
Updated: 13/11/2026
Silicon photonics — waveguides, ring resonators, grating couplers
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: 1.72 ± 0.21 dB/cm (0.50 µm strip, air-clad).
Clean → Spin coat → Bake → EBL exposure → Develop → (Reflow) → Si etch → Resist strip → Inspect → Dice
|
Step 1 — Substrate clean 10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N2 dry. 5 min dehydration bake at 180 °C, then 5 min O2 plasma (200 W, 100 sccm O2, 10 mTorr).
Step 2 — Resist coating Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N2 before dispensing.
Step 3 — Pre-exposure bake 180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI").
Step 4 — EBL exposure Expose at 100 kV as two passes from one BEAMER flow (see EBL data preparation below):
Step 5 — Development 60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N2 dry.
Step 6 — Resist reflow (optional) 135–140 °C for 60–120 s, to smooth the resist sidewall before etching.
Step 7 — Si etch Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see Si etch sequence below). Si : ZEP selectivity is ~1.55 : 1.
Step 8 — Resist removal Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O2 plasma at 200 W.
Step 9 — Inspection Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.
Step 10 — Dicing Coat with AZ protective resist, dice, then solvent clean as in Step 1.
|
Facilities used
Key instruments
Typical resists
Wafer stack
Key numbers
|
EBL data preparation (BEAMER)
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.
- Waveguide bias: +7 nm per edge.
- Sleeve (fine): 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.
- Bulk (coarse): band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.
- Assist: waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.
- Fields: 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.
- PEC: Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).
Si etch sequence
Every etch session conditions the chamber first, then runs a two-step etch.
- O2 chamber clean: 5 min minimum, typically 10 min.
- SF6/O2 clean: 5 min.
- Si precondition: 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.
- Load sample on a carrier wafer with oil.
- Stabilise (strike) step: ~6 s; etches ~38 nm, so include it in the depth budget.
- Main etch: ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.
Process flow website
Interactive version of this process flow: Photonics process flow