Photonics: Difference between revisions

From CMM Wiki
Jump to navigationJump to search
m Updated with expanding sections for BEAMER and silicon etching.
Line 1: Line 1:
== Photonics — Si photonics, metalenses, integrated photonics ==
== Photonics — Si photonics, metalenses, integrated photonics ==
''Nanofabrication workflows for integrated photonic devices.''
''Nanofabrication workflows for integrated photonic devices.''
[[File:Photonic circuit process flow v2.png|none|left|Typical process flow of a photonic integrated circuit]]


=== 220nm Silicon-on-Insulator Photonics - Standard Process ===
=== 220nm Silicon-on-Insulator Photonics - Standard Process ===

Revision as of 12:58, 17 November 2026

Photonics — Si photonics, metalenses, integrated photonics

Nanofabrication workflows for integrated photonic devices.

Typical process flow of a photonic integrated circuit
Typical process flow of a photonic integrated circuit

220nm Silicon-on-Insulator Photonics - Standard Process

Updated: 13/11/2026

Silicon photonics — waveguides, ring resonators, grating couplers

EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: 1.72 ± 0.21 dB/cm (0.50 µm strip, air-clad).

220 nm SOI standard process flow
220 nm SOI standard process flow

Step 1 — Substrate clean

10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N2 dry. 5 min dehydration bake at 180 °C, then 5 min O2 plasma (200 W, 100 sccm O2, 10 mTorr).

  • CMM — fume hood and sonicator
  • CMM — Diener plasma cleaner

Step 2 — Resist coating

Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N2 before dispensing.

  • CMM — CEE Apogee spin coater

Step 3 — Pre-exposure bake

180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI").

  • Hotplate
  • Filmtek

Step 4 — EBL exposure

Expose at 100 kV as two passes from one BEAMER flow (see EBL data preparation below):

  • Fine (sleeve): 0.5 nA, 260 µC/cm², 2 nm beam step
  • Coarse (bulk): 20 nA, 280 µC/cm², 10 nm beam step
  • CMM — Raith EBPG5150 (100 kV)
  • Process flow PDF: SiCOI litho

Step 5 — Development

60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N2 dry.

  • CMM — fume hood

Step 6 — Resist reflow (optional)

135–140 °C for 60–120 s, to smooth the resist sidewall before etching.

  • Hotplate

Step 7 — Si etch

Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see Si etch sequence below). Si : ZEP selectivity is ~1.55 : 1.

  • ANFF-Q — Oxford ICP-RIE

Step 8 — Resist removal

Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O2 plasma at 200 W.

  • CMM — fume hood, Diener plasma cleaner

Step 9 — Inspection

Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.

  • Optical microscope
  • CMM — Dektak; ANFF-Q — KLA profiler
  • CMM — eLINE Plus (CD-SEM)

Step 10 — Dicing

Coat with AZ protective resist, dice, then solvent clean as in Step 1.

  • Sawatec spin coater (protective coat)
  • Accretech dicing saw

Facilities used

  • CMM (Hawken) — clean, coat, EBL, metrology
  • ANFF-Q (AIBN) — etch, depth profiling

Key instruments

  • Raith EBPG5150 (100 kV EBL)
  • BEAMER (EBL data preparation)
  • eLINE Plus (CD-SEM)
  • Oxford ICP-RIE
  • Diener plasma cleaner
  • CEE Apogee spin coater
  • Filmtek (film thickness)
  • Dektak / KLA (step height)
  • Accretech dicing saw

Typical resists

  • ZEP520A — positive tone (standard process)
  • HSQ 6% — negative tone hard mask (alternative; not yet part of the standard process)

Wafer stack

  • Si 220 ± 10 nm
  • BOX 3000 ± 50 nm
  • Handle 725 ± 25 µm
  • Cladding: air

Key numbers

  • Loss: ~1.7–2.3 dB/cm (0.50 µm)
  • Etch rate: ~5.9 nm/s
  • Etch depth: 228–232 nm
  • Si : ZEP selectivity: 1.55 : 1
EBL data preparation (BEAMER)

Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.

  • Waveguide bias: +7 nm per edge.
  • Sleeve (fine): 150 nm band around the waveguide plus 150 nm overlap into the bulk; 2 nm beam step; smooth shot filling.
  • Bulk (coarse): band out to 5 µm from the waveguide; 10 nm beam step; high-resolution shot filling.
  • Assist: waveguide + 5 µm; used only to place write fields along the waveguides, never exposed.
  • Fields: 1040 µm main fields, 10 µm overlap on the fine layer; conventional fracturing.
  • PEC: Monte Carlo point-spread function for 100 kV on ZEP / 220 nm Si / 3 µm BOX (β 30, η 0.6).
Si etch sequence

Every etch session conditions the chamber first, then runs a two-step etch.

  1. O2 chamber clean: 5 min minimum, typically 10 min.
  2. SF6/O2 clean: 5 min.
  3. Si precondition: 5 min of the etch recipe on a carrier. Its DC bias predicts the etch bias to ~3 V; note it before loading.
  4. Load sample on a carrier wafer with oil.
  5. Stabilise (strike) step: ~6 s; etches ~38 nm, so include it in the depth budget.
  6. Main etch: ~5.9 nm/s; 32 s for the full 220 nm etch, 6–7 s for a 70–80 nm shallow etch.

Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded.