Photonics
Photonics — Si photonics, metalenses, integrated photonics
Nanofabrication workflows for integrated photonic devices.
220nm Silicon-on-Insulator Photonics - Standard Process
Updated: 13/11/2026
Silicon photonics — waveguides, ring resonators, grating couplers
EBL-defined silicon-on-insulator (SOI) strip waveguides in 220 nm Si on 3 µm buried oxide: one full etch, air-clad. Waveguides are typically 0.5–1.0 µm wide; design minimum 100 nm width and 150 nm gap. Best propagation loss to date: 1.72 ± 0.21 dB/cm (0.50 µm strip, air-clad).

|
Step 1 — Substrate clean 10 min DMSO at 70 °C; acetone rinse; 5 min acetone with sonication (40 %); acetone rinse; 2 min IPA with sonication (40 %); IPA rinse; N2 dry. 5 min dehydration bake at 180 °C, then 5 min O2 plasma (200 W, 100 sccm O2, 10 mTorr).
Step 2 — Resist coating Spin 350 nm ZEP520A at 6000 rpm for 60 s. Use ~0.5 mL for 15–20 mm dies and 1.25–1.5 mL for a 4″ wafer. Let the resist reach room temperature first, and blow the pipette tip with N2 before dispensing.
Step 3 — Pre-exposure bake 180 °C for 5 min. Measure the resist thickness on the Filmtek (recipe "ZEP520A on SOI").
Step 4 — EBL exposure Expose at 100 kV as two passes from one BEAMER flow (see EBL data preparation below):
Step 5 — Development 60 s in ZED-N50 at room temperature with a gentle swirl every 10 s; 15 s in IPA; N2 dry.
Step 6 — Resist reflow (optional) 135–140 °C for 60–120 s, to smooth the resist sidewall before etching.
Step 7 — Si etch Full etch through the 220 nm Si to the buried oxide: 32 s main step at ~5.9 nm/s, after a chamber clean and Si precondition (see Si etch sequence below). Si : ZEP selectivity is ~1.55 : 1.
Step 8 — Resist removal Repeat the Step 1 solvent clean (DMSO, acetone, IPA), then 5 min O2 plasma at 200 W.
Step 9 — Inspection Optical microscope check, etch depth by stylus profiler, and CD-SEM of critical features.
Step 10 — Dicing Coat with AZ protective resist, dice, then solvent clean as in Step 1.
|
Facilities used
Key instruments
Typical resists
Wafer stack
Key numbers
|
| EBL data preparation (BEAMER) |
|---|
|
Each layout is split into a fine and a coarse exposure. The fine beam writes a narrow band that sets the waveguide sidewall; the fast coarse beam clears the rest of the 5 µm trench.
|
| Si etch sequence |
|---|
|
Every etch session conditions the chamber first, then runs a two-step etch.
Recipe set-points (gases, flows, ICP and RF power, pressure, table temperature) are still to be recorded. |